An isolation kit puts PTFE, an elastomer seal, a glass-reinforced laminate retainer and a metal core in contact with the same line fluid. A material that survives the medium but not the temperature, or survives both but not as part of the stack, is how a joint fails six weeks after start-up. This chart rates every material Protek wets — along with the sleeve and washer compounds that sit outside the seal — from A to X so you can screen a service before you specify it.
Seal elements — FKM and EPDM shown for reference; seal compound availability by product – confirm with Protek.
| Medium | Seal elements | Retainers & washers | Sleeves | Core metallurgy | ||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| 44 media listed | PTFE | Nitrile (NBR) | FKM (Viton®-type) | EPDM | G10 | G11 | Phenolic | Mylar (PET) | Nomex | Mineral-filled Nylon | 316 SS | Duplex 2205 | Super Duplex 2507 | Alloy 625 |
| Water, fresh/cooling | A | A | A | A | A | A | B | A | A | B | A | A | A | A |
| Seawater / brine | A | A | A | A | A | A | B | A | B | B | B1 | B | A | A |
| Produced water (H2S/CO2/chlorides)2 | A | B | A | C | A | A | C | A | B | C | C | B | A | A |
| Steam (to 300°F)3 | A | C | C | A | C | C | C | X | C | X | A | A | A | A |
| Crude oil, sweet | A | A | A | X | A | A | A | A | A | A | A | A | A | A |
| Crude oil, sour (H2S)4 | A | C | A | X | A | A | B | A | A | B | B | A | A | A |
| Natural gas, dry | A | A | A | C | A | A | A | A | A | A | A | A | A | A |
| Natural gas, wet/sour5 | A | B | A | X | A | A | B | A | A | B | B | A | A | A |
| Hydrogen sulfide gas6 | A | C | B | A | A | A | B | A | A | B | B | B | A | A |
| Carbon dioxide, dry | A | A | A | B | A | A | A | A | A | A | A | A | A | A |
| Hydrogen gas | A | A | A | A | A | A | A | A | A | A | A | B7 | B8 | A |
| Nitrogen / air | A | A | A | A | A | A | A | A | A | A | A | A | A | A |
| Methanol | A | B | C | A | A | A | B | A | A | B | A | A | A | A |
| Ethanol | A | B | B | A | A | A | A | A | A | B | A | A | A | A |
| Glycol (MEG/TEG) | A | A | A | A | A | A | A | A | A | A | A | A | A | A |
| Diesel / jet fuel | A | A | A | X | A | A | A | A | A | A | A | A | A | A |
| Gasoline | A | B | A | X | A | A | A | A | A | A | A | A | A | A |
| Hexane / aliphatic hydrocarbons | A | A | A | X | A | A | A | A | A | A | A | A | A | A |
| Toluene / xylene (aromatics) | A | X | A | X | A | A | A | B | A | A | A | A | A | A |
| Benzene | A | X | A | X | A | A | A | B | A | A | A | A | A | A |
| Acetone / ketones | A | X | X | A | A | A | B | B | A | A | A | A | A | A |
| Chlorinated solvents | A | X | B | X | B | B | B | C | A | B | A | A | A | A |
| Hydraulic oil, mineral | A | A | A | X | A | A | A | A | A | A | A | A | A | A |
| Phosphate ester fluids | A | X | X | A | A | A | A | B | A | B | A | A | A | A |
| Amines (MEA/DEA/MDEA) | A | B | X | A | B | B | C | X | B | B | A | A | A | A |
| Ammonia, anhydrous | A | B | X | A | B | B | C | C | B | B | A | A | A | A |
| Hydrochloric acid, dilute (<10%) | A | C | A | B | B | B | B | B | C | X | X | C | B | B |
| Hydrochloric acid, concentrated | A | X | B | C | C | C | C | C | X | X | X | X | X | C |
| Sulfuric acid, dilute (<10%) | A | C | A | A | B | B | B | A | C | X | B | A | A | A |
| Sulfuric acid, concentrated (93–98%) | A | X | A | X | X | X | X | X | X | X | B | B | B | B |
| Nitric acid, dilute (<10%) | A | X | B | C | C | C | C | B | C | X | A | A | A | A |
| Nitric acid, concentrated | A | X | C | X | X | X | X | X | X | X | B | B | B | B |
| Phosphoric acid | A | C | A | A | B | B | B | B | C | X | A | A | A | A |
| Hydrofluoric acid | A | X | B | X | X | X | X | C | X | X | X | X | X | C |
| Acetic acid | A | C | C | A | B | B | B | B | B | X | A | A | A | A |
| Citric / organic acids, dilute | A | A | A | A | A | A | A | A | A | B | A | A | A | A |
| Sodium hydroxide, dilute (<20%) | A | B | C | A | C | C | X | X | C | A | A9 | A | A | A |
| Sodium hydroxide, 50% | A | C | A | X | X | X | X | X | C | B | B10 | B | A | A |
| Sodium hypochlorite (bleach) | A | X | A | B | C | C | C | B | C | X | X | C | B | B |
| Chlorine, wet | A | X | B | C | C | C | X | C | X | X | X | X | C | C |
| Chlorine, dry gas | A | X | A | C | B | B | C | B | C | X | B | B | B | A |
| Hydrogen peroxide, dilute | A | C | A | B | B | B | C | B | C | X | A | A | A | A |
| Ozone / weathering | A | C | A | A | A | A | A | A | A | A | B | A | A | A |
| LNG / cryogenic (to −260°F) | A | X | X | X | B | B | C | B | B | C | A | X11 | X12 | A |
- 1.Seawater / brine — 316 SS: crevice/pitting risk in stagnant or warm seawater
- 2.Produced water (H2S/CO2/chlorides): Metals must meet NACE MR0175/ISO 15156 limits.
- 3.Steam (to 300°F): Laminates and PET limited by temperature and hydrolysis.
- 4.Crude oil, sour (H2S): Metals must meet NACE MR0175/ISO 15156 limits.
- 5.Natural gas, wet/sour: Metals must meet NACE MR0175/ISO 15156 limits.
- 6.Hydrogen sulfide gas: Metals must meet NACE MR0175/ISO 15156 limits.
- 7.Hydrogen gas — Duplex 2205: hydrogen embrittlement risk under cathodic protection
- 8.Hydrogen gas — Super Duplex 2507: hydrogen embrittlement risk under cathodic protection
- 9.Sodium hydroxide, dilute (<20%) — 316 SS: caustic stress-corrosion cracking risk at elevated temperature
- 10.Sodium hydroxide, 50% — 316 SS: caustic stress-corrosion cracking risk at elevated temperature
- 11.LNG / cryogenic (to −260°F) — Duplex 2205: duplex steels lose toughness below about −50°F
- 12.LNG / cryogenic (to −260°F) — Super Duplex 2507: duplex steels lose toughness below about −50°F
General guidance compiled from published polymer, elastomer and alloy compatibility references. Ratings change with temperature, concentration, pressure and combined media. Verify for your service conditions; contact Protek Engineering for a written recommendation.
Send the medium, concentration, temperature and pressure and Protek Engineering will confirm the seal compound, retainer and core for your line.
- Parker O-Ring Handbook ORD 5700
- Cole-Parmer Chemical Compatibility Database
- NEMA LI 1 (industrial laminates)
- NACE MR0175/ISO 15156
Chemical compatibility questions
How do I read the A / B / C / X ratings?
+−
A means excellent — no meaningful effect at ambient temperature. B means good, with a minor effect such as slight swelling or discoloration that does not change the seal. C means fair or limited service: test the actual medium or consult Protek before specifying it. X means not recommended. Every rating is for ambient temperature unless the medium name states otherwise.
Why are the products rated per material and not per part number?
+−
An isolation kit is a stack of dissimilar materials. The wetted set is the gasket and retainer face plus, on metal-cored products, the core. Scout uses an NBR seal with a phenolic retainer, Delta uses a G10 or G11 retainer with the seal compound you select, and Ranger and Ranger FS use a PTFE seal with a G10 or G11 retainer and a 316 SS, duplex, super duplex or Alloy 625 core. The product column shows the worst rating of those wetted materials, and the sleeve and washer materials — Mylar, Nomex, mineral-filled nylon — are shown for reference because they are not wetted.
Does temperature change the rating?
+−
Yes, sometimes dramatically. Pet and laminate materials are limited by temperature and hydrolysis, so steam service is the clearest example. Acids, caustics and solvents generally become more aggressive as temperature rises, and elastomer swell increases with concentration. Use this chart to screen candidates, then confirm with Protek Engineering for the operating temperature and concentration of your line.
What if my line combines several media?
+−
Combined media are not the same as either medium alone. A produced-water stream carrying H2S, CO2 and chlorides is more aggressive than any single row suggests, and a solvent-wet gas can strip swell out of an elastomer that is fine in the neat liquid. Rate the most aggressive constituent and confirm the combination with a written recommendation.
Do these ratings cover sour service metallurgy?
+−