ISOLATION GASKET
MATERIAL PROPERTIES
An isolation joint is a stack of four different material families: a dielectric retainer, a seal element, insulating sleeves and washers, and a metal core. This table puts their typical dielectric strength, compressive strength, temperature capability and alloy resistance side by side, so you can see what each layer contributes — and which one becomes the limit.
Pick up to three materials for side-by-side bars and a property table.
| Property | G10 glass-epoxy | G11 glass-epoxy |
|---|---|---|
| Standard / UNS | NEMA G10 / MIL-I-24768/2 | NEMA G11 |
| Dielectric strength | 800–800 V/mil | 400–600 V/mil |
| Compressive strength | 65,000 psi | 60,000 psi |
| Max temperature | 284°F (140°C) | 285–300°F (140–150°C) |
| Water absorption | ≤0.25% | ≤0.25% |
| PREN | — | — |
| Min yield (annealed plate) | — | — |
| Notes | The standard dielectric retainer: high compressive strength, low moisture pick-up, good electrical strength in the dry condition. | Better strength retention at temperature than G10, with a slightly lower dielectric strength. |
16 materials available to compare — typical values only.
| Material | Standard / UNS | Dielectric (V/mil) | Compressive (psi) | Max temp | Water | PREN | Yield (ksi) | Notes |
|---|---|---|---|---|---|---|---|---|
| Dielectric laminates | ||||||||
| G10 glass-epoxy | NEMA G10 / MIL-I-24768/2 | 800–800 | 65,000 | 284°F (140°C) | ≤0.25% | — | — | The standard dielectric retainer: high compressive strength, low moisture pick-up, good electrical strength in the dry condition. |
| G11 glass-epoxy | NEMA G11 | 400–600 | 60,000 | 285–300°F (140–150°C) | ≤0.25% | — | — | Better strength retention at temperature than G10, with a slightly lower dielectric strength. |
| Phenolic laminate (paper / fabric) | NEMA XXX / CE | 300–750 | 35,000 | 250°F (121°C) | Higher moisture absorption | — | — | Economical retainer used on Scout. Good compressive strength for the cost; moisture absorption is higher than the epoxies. |
| G3 glass-phenolic | NEMA G3 | 300–450 | 55,000 | 250°F (121°C) | Higher moisture absorption | — | — | Glass-reinforced phenolic: stronger than a plain paper phenolic, with similar temperature limits. |
| G7 glass-silicone | NEMA G7 | 250–400 | — | 425°F (218°C) | — | — | — | Silicone binder gives the highest temperature capability of the laminates, with high arc resistance and lower mechanical strength. |
| Films, papers & nylon | ||||||||
| Mylar (PET film) | PET film | 7000–7000 | — | 300°F (150°C) | — | — | — | Very high dielectric strength per unit thickness. Used as an economical sleeve; limited by temperature and hydrolysis in steam. |
| Nomex (aramid paper) | Aramid paper | 400–900 | — | 428°F (220°C) | — | — | — | High-temperature sleeve material with good dielectric strength that varies strongly with wall thickness. |
| Mineral-filled nylon | Mineral-filled PA | 400–600 | — | 220°F | Absorbs moisture | — | — | Tough and abrasion resistant, but absorbs moisture — dimensional change and loss of electrical strength in wet service. |
| Seal elements | ||||||||
| PTFE | Virgin / filled PTFE | 500–500 | — | −328°F to +500°F | None | — | — | Near-universal chemical resistance and the widest temperature range. Cold flows under load, which is why Protek retains it mechanically. |
| Nitrile (NBR) | — | — | — | −40°F to +250°F | — | — | — | Good resistance to oils and fuels; poor resistance to ozone, ketones and strong acids. |
| FKM (Viton®-type) | — | — | — | −15°F to +400°F | — | — | — | Fluorocarbon with the broadest chemical and temperature range of the elastomers; not for ketones or amines. |
| EPDM | — | — | — | −60°F to +300°F | — | — | — | Excellent water, steam and ozone resistance; swells badly in hydrocarbons and oils. |
| Core metallurgy | ||||||||
| 316 / 316L stainless | UNS S31600 / S31603 | — | — | — | — | ≈24 | 30 | Standard core. NACE MR0175/ISO 15156 applies within the standard's environmental limits. |
| Duplex 2205 | UNS S31803 / S32205 | — | — | — | — | ≈35 | 65 | Roughly twice the yield of 316 with better chloride resistance. Duplex steels lose toughness below about −50°F. |
| Super Duplex 2507 | UNS S32750 | — | — | — | — | ≈42 | 80 | Higher PREN and yield than 2205 for severe chloride service. The same low-temperature toughness limit applies. |
| Alloy 625 | UNS N06625 | — | — | — | — | ≈51 | 60 | Nickel-chromium-molybdenum alloy for the most aggressive service; acceptable to high H2S partial pressures under NACE MR0175. |
Typical values for comparison, not specifications. Actual properties vary by manufacturer, thickness, construction and test method — contact Protek for the data sheet of the material on your order.
Sources: NEMA LI 1; Manufacturer data sheets (e.g. Atlas Fibre G-10); DuPont Mylar / Nomex literature; ASTM A240 / B443.
Alloy metallurgy for sour service is governed by NACE MR0175/ISO 15156, and duplex grades lose toughness below about −50°F. For high-temperature service, contact Protek for the high-temperature laminate selection.
Build the kit for your flange and download the drawing, or send the service conditions to Protek Engineering for a written recommendation and quote.
Material property questions
Are these values specifications?
+−
No. They are typical values for comparison, collected from NEMA LI 1, manufacturer data sheets and alloy standards. Actual properties vary with manufacturer, construction, thickness and test method, so contact Protek for the data sheet of the material on your order.
Why does the product temperature rating differ from the laminate rating?
+−
The product rating is the published service range of the assembled Protek gasket, which is set by the seal system and the retained core, not by the retainer laminate alone. Where a service sits above the typical laminate temperature, contact Protek for the high-temperature laminate selection and a written recommendation.
What does PREN tell me?
+−
The pitting resistance equivalent number — roughly %Cr + 3.3 × %Mo + 16 × %N — ranks an alloy's resistance to chloride pitting. 316 is around 24, duplex 2205 about 35, super duplex 2507 about 42 and Alloy 625 about 51. Higher is better, but PREN does not cover crevice geometry, temperature or H2S.
Why is cold flow a problem for PTFE?
+−
PTFE creeps under sustained compressive load, so a plain PTFE gasket loses bolt load over time. Protek retains the PTFE seal mechanically in a groove and carries the bolt load through a metal core and a dielectric retainer, so the PTFE only has to seal, not support the joint.