Engineering Tools

GALVANIC CORROSION CHART
& FLANGE ISOLATION CHECKER

Bolt a carbon steel flange to a stainless one and the studs quietly make them a single piece of metal. In seawater, produced water or wet soil that couple corrodes the less noble side — usually in the crevice at the gasket face, where nobody sees it until the joint leaks. Pick the two metals and the environment below to rate the couple, then look up the potentials that drive it.

Flange isolation checker
Galvanic risk
Severe
Potential difference
0.57 V
Anode — corrodes
Carbon steel
Cathode — protected
316 stainless
Carbon steel −0.65 V · 316 stainless −0.07 V · basis: seawater series (midpoint)
Weld-neck joint, half section
Carbon steel — ANODE316 stainless — CATHODEISOLATION KIT — gasket + full-length sleeves + isolating washersbreak the metal path123456789101Weld-neck flange (anode side)2Weld-neck flange (cathode side)3Raised face4Isolation gasket (Type F)5Isolating sleeve (full length)6Isolating washer7Steel washer8Heavy hex nut9Stud bolt (2 threads proud)10Pipeionic current in electrolyteblocked electronic path at every metal interfaceDETAIL A — 3×Raised face step, gasket and the face gap outside the RF.RF step 0.060″ · gap outside RF 0.370″Gasket 7.00″ OD × 0.250″ thick, bore 4.036″Proportions per ASME B16.5 Class 300 NPS 4 weld-neck; illustration only.
  • Immersion in an electrolyte makes the couple active; stagnant or warm seawater also drives crevice corrosion.

Severe galvanic risk — a full flange isolation kit is mandatory (gasket + full-length sleeves + double isolating washers). Suggested: Protek Ranger FS; coat the cathode, never just the anode, and verify isolation per NACE SP0286.

Galvanic series in flowing seawater

Potentials in volts against a saturated calomel electrode, most active at the top. Two alloys far apart on this list form a strong couple; two in the same band are effectively safe together.

Galvanic series — flowing seawater, V vs SCE
−1.60−1.20−0.80−0.40+0.00+0.40
−1.63…−1.60
−1.03…−0.98
−0.90…−0.70
−0.76…−0.70
−0.72…−0.60
−0.70…−0.60
−0.54…−0.43
−0.40…−0.30
−0.40…−0.30
−0.36…−0.28
−0.34…−0.25
−0.27…−0.24
−0.35…−0.20
−0.28…−0.21
−0.25…−0.19
−0.22…−0.13
−0.20…−0.10
−0.14…−0.09
−0.14…−0.04
−0.07
−0.15…+0.00
−0.01
−0.05…+0.06
−0.04…+0.10
−0.04…+0.10
+0.18…+0.25
+0.20…+0.30

Rotate your device or widen the window for labels.

MaterialActive end (V)Noble end (V)Midpoint (V)
Magnesium-1.63-1.60-1.61
Zinc / galvanized steel-1.03-0.98-1.00
Aluminum alloys-0.90-0.70-0.80
Cadmium-0.76-0.70-0.73
Cast iron-0.72-0.60-0.66
Carbon & low-alloy steel-0.70-0.60-0.65
300-series stainless (active — crevices / stagnant)-0.54-0.43-0.48
Aluminum bronze-0.40-0.30-0.35
Brasses-0.40-0.30-0.35
Copper-0.36-0.28-0.32
Admiralty brass-0.34-0.25-0.30
Silicon bronze-0.27-0.24-0.26
400-series stainless (passive)-0.35-0.20-0.28
90-10 copper-nickel-0.28-0.21-0.24
Lead-0.25-0.19-0.22
70-30 copper-nickel-0.22-0.13-0.17
17-4 PH stainless-0.20-0.10-0.15
Silver-0.14-0.09-0.12
Monel 400-0.14-0.04-0.09
Duplex 2205-0.07-0.07-0.07
316 SS (passive)-0.150.00-0.07
Super duplex 2507-0.01-0.01-0.01
Titanium-0.050.060.00
Alloy 625-0.040.100.03
Hastelloy C-276-0.040.100.03
Platinum0.180.250.21
Graphite0.200.300.25

300-series stainless steels in low-velocity or poorly aerated water, or inside crevices, may become active and show potentials near −0.5 V.

Passive alloys covered by marine biofilms may shift to +0.3 to +0.4 V.

Flowing seawater at ambient temperature — S.C. Dexter, University of Delaware Sea Grant; ASTM G82; Titanium Information Group (duplex values).

Anodic index — non-immersion service

Where the joint is not immersed — atmospheric, buried or dry indoor service — the checker ranks the couple on the anodic index instead of the seawater series. It is a relative table, so only the difference matters.

Anodic Index (MIL-F-14072 Table VI–derived design rule)
MetalVolts
Gold0.00
Rhodium0.05
Silver / Monel / high nickel-copper0.15
Nickel, titanium0.30
Copper, low brass/bronze, nickel-chromium alloys0.35
Brass & bronze0.40
High brass & bronze0.45
18% Cr stainless (300-series)0.50
Chromium plate, tin plate, 12% Cr stainless0.60
Tin-lead solder0.65
Lead0.70
2000-series aluminum0.75
Carbon & low-alloy steel, cast iron0.85
Other wrought / cast aluminum0.90
Cast aluminum (non-silicon), cadmium0.95
Hot-dip galvanized1.20
Zinc / zinc plate1.25
Magnesium1.75
Rule of thumb — max difference
Harsh / marine / outdoor0.15 V
Normal indoor0.25 V
Controlled atmosphere0.50 V

Rule of thumb only — it is not part of MIL-STD-889. Use the potential difference for the specific environment.

What galvanic corrosion actually is

Every alloy sits at a natural potential in an electrolyte. Join two of them electrically and the one with the more negative potential becomes the anode: it gives up metal ions, and the cathodic reaction — oxygen reduction in neutral water, hydrogen evolution in acids — runs on the more noble surface. The metals do not have to touch the fluid in the same way; the circuit only needs a continuous metal path and a continuous electrolyte path. In a bolted flange, the studs are the metal path.

Why flanges and cathodic protection need isolation

A cathodically protected pipeline sitting at a few hundred millivolts below its free potential will try to protect everything it is connected to. If an unprotected flange, a wellhead or a small-diameter branch is bonded through its bolting, the CP system feeds it as well: current drains away, the protected line is under-protected, and the stray current accelerates attack on the neighbouring structure. Isolation stops the drain and keeps each system on its own potential.

Sleeves and washers do the work, not the gasket

An isolating gasket alone isolates nothing: the studs pass straight through the bolt holes and short the two flange faces together. Full-length insulating sleeves line the bolt holes through the full flange thickness, and isolating washers under both nuts and both flange faces keep the nut from contacting the flange. A conventional steel washer on one side defeats the whole kit.

Coatings: protect the cathode, not just the anode

Painting the anode is the intuitive move and usually the wrong one. A coating has holidays — pinholes and scratches — and if only the anode is coated, all of the galvanic current concentrates on that small bare area, so pitting gets worse. Coat the cathode to reduce the cathodic reaction, leave the anode bare or coat both, and never treat a coating as electrical isolation.

The area ratio decides how fast it bites

A small anode facing a large cathode is the dangerous geometry: all the cathodic current is discharged into a small area of metal, so penetration rate climbs. A stainless flange against a carbon steel spool is worse than the potentials alone suggest, while a large carbon steel flange against a small stainless fitting is comparatively benign. The checker raises the risk one level whenever the cathode is much larger than the anode.

Proving the isolation after assembly

NACE SP0286 covers the electrical isolation of cathodically protected piping. Measure across the joint with a calibrated isolation tester or megohmmeter once the flange is fully torqued, and record the reading on the joint record. If the resistance is effectively zero, a sleeve is short, a washer is trapped, or a metallic component has been substituted — all of which happen in the field more often than the potential difference does.

FAQ

Galvanic corrosion questions

Why do dissimilar-metal flanges need isolation?

+

Two different alloys joined by a bolted flange are electrically connected through the studs and nuts. Add an electrolyte — seawater, produced water, even wet soil — and the less noble alloy becomes the anode and corrodes, often in a tight crevice at the gasket face where it cannot be seen. A full isolation kit breaks that circuit: an isolating gasket between the faces, full-length sleeves through the bolt holes and isolating washers under both nuts.

What is the difference between the galvanic series and the anodic index?

+

The galvanic series lists actual measured potentials for alloys in flowing seawater against a saturated calomel electrode. The anodic index is a design table of relative potentials against gold, used when you are not in seawater and just need a consistent ranking. Under immersion the seawater series is the better basis; in atmospheric or buried service the anodic index is used. This tool switches basis automatically with the environment you select.

How much potential difference is acceptable?

+

As a rule of thumb, keep the couple below 0.15 V in harsh, marine or outdoor service, below 0.25 V indoors and below 0.50 V only in a controlled, dry atmosphere. That rule is not drawn from MIL-STD-889, which defines test methods rather than limits. Exceeding it does not mean the joint instantly fails, it means the anode needs protection — which is what an isolation kit provides.

Why does the area ratio matter so much?

+

Corrosion rate is driven by current density at the anode. A large cathode feeding a small anode concentrates all of the cathodic current into a small area, so a stainless body against a carbon steel flange bolt-hole strip can pit through quickly, while the reverse pairing is far more forgiving. That is why the checker raises the risk one level whenever the cathode is much larger than the anode.

How do I prove the joint is actually isolated?

+

After assembly, measure across the joint with a calibrated isolation tester or megohmmeter per NACE SP0286 and record the reading. A dead short means a sleeve is missing, a washer is trapped under a nut incorrectly, or a metallic gasket or spiral wound washers were used instead of an isolating set. Coatings do not count as isolation, and coating only the anode usually makes pitting worse by concentrating attack at coating defects.